Interdur 8844 High Solids Epoxy belongs to Epoxy. For the protection of steel structures in all corrosive environments, including splash zones of offshore structures, under-deck and above-water areas, pile structures, paper mills, bridges and chemical plants. A high solids, low VOC, high-build epoxy primer/intermediate or topcoat, incorporating chemical-resistant, high aspect ratio glass flake to enhance product durability, abrasion resistance and corrosion resistance. When Interdur 8844 is applied by brush or roller, multiple coats are necessary to achieve the specified total system dry film thickness. Parameters on this page: volume solids 87% (± 2%), dry film thickness 200–500 µm (8–20 mils), theoretical spreading rate 2.90 m²/L.
Parameter source: AKZONOBEL original technical data sheet (TDS) "Interdur 8844 High Solids Epoxy"; values such as spreading rate are converted from TDS parameters and are for selection reference only.
The above content is compiled from the manufacturer's datasheet and this site's parameter tables. For selection, coating systems and lead times, pleaseContact Usfor confirmation.
This page carries the full TDS for this product, translated from the manufacturer's original document. No file download is needed; for an original-language copy, send an enquiry.
| Volume Solids | 87% ( ± 2%) |
|---|---|
| Dry Film Thickness | 200–500 µm (8–20 mil) |
| Theoretical Spreading Rate | 2.90 m²/L |
| VOC | 1.90 lb/gal (228 g/L) US EPA Method 24 15… |
| Density / Specific Gravity | 1.63 kg/L (13.6 lb/gal) |
| Number of Components | — |
| Thinner | Recommended maximum thinning ratio not to exceed 5%. Normally no thinning is required. |
| Mixing Ratio | 4 parts : 1 part (by volume) |
| Gloss |
For more Q&A on selection, application, acceptance and defect diagnosis, seeFAQsection.
A high solids, low VOC, high-build epoxy primer/intermediate or topcoat, incorporating chemical-resistant, high aspect ratio glass flake to enhance product durability, abrasion resistance and corrosion resistance.
For the protection of steel structures in all corrosive environments, including splash zones of offshore structures, under-deck and above-water areas, pile structures, paper mills, bridges and chemical plants.
Provides excellent long-term corrosion resistance for new construction and maintenance.
INTERDUR Colour White 8844
| Gloss | |
|---|---|
| Volume Solids | 87% (± 2%) |
| Typical thickness | Dry film thickness 200–500 µm (8–20 mils) corresponds to wet film thickness 230–575 µm (9.2–23 mils) |
| Theoretical Spreading Rate | At 300 µm dry film thickness and the stated volume solids, 2.90 m²/L; at 12 mils dry film thickness and the stated volume solids, 116 ft²/US gal |
| Practical Spreading Rate | Allowing for a suitable loss factor |
| Application Methods | Air spray, suitable for airless spray, brush, roller. Drying time; self-recoat interval |
| Temperature | Surface Dry | Hard Dry | Minimum | Maximum |
| 10°C (50°F) | 14 h | 24 h | 14 days | |
| 15°C (59°F) | 10 h | 18 h | 10 days | |
| 25°C (77°F) | 4 h | 8 h | 7 days | |
| 40°C (104°F) | 90 min | 3 h | 5 days | |
| Flash point (typical) | Component A 30 °C (86 °F); Component B 44 °C (111 °F); after mixing 33 °C (91 °F) |
|---|---|
| Product weight | 1.63 kg/L (13.6 lb/gal) |
| Volatile Organic Compounds | 1.90 lb/gal (228 g/L) US EPA Method 24; 159 g/L Chinese National Standard GB/T 23985-2009; coating hazard GB 30981.2-S-Pb≤1000-NC complies with GB 30981.2-2025. For more detailed information, please refer to the "Product Characteristics" section. |
The performance of this product depends on the degree of surface preparation. All surfaces to be coated must be clean, dry and free of contamination. Before painting, all surfaces must be assessed in accordance with ISO 8504:2000
| assessed and prepared in accordance with the standard. | Accumulated dirt and soluble salts must be removed. Dirt is generally brushed off with a dry bristle brush. Soluble salts should be washed off with fresh water. |
|---|
Blast cleaning: For immersion service, Interdur 8844 must be applied to surfaces blast cleaned to Sa2½ (ISO 8501-1:2007) or SSPC SP10. However, for atmospheric exposure, Interdur 8844 should be applied to surfaces blast cleaned to Sa2½ (ISO 8501-1:2007) or at least SSPC SP6.
Surface defects exposed by blast cleaning must be ground, filled or treated by a suitable method.
Recommended angular surface profile of 50–75 µm (2–3 mils).
| Mixing | This product is supplied in two containers forming one unit. Mix the two components in the specified ratio in one operation. Once mixed, use within the specified pot life. |
|---|
(1) Stir the base (Component A) with a power mixer.
(2) Mix all of the curing agent (Component B) with the base (Component A) and stir thoroughly with a power mixer.
| Mixing ratio | 4 parts : 1 part (by volume) |
|---|
| Pot life | 10°C (50°F) | 15°C (59°F) | 25°C (77°F) | 40°C (104°F) |
| 3 h | 2 h | 90 min | 45 min |
| Suitable for airless spray | Recommended nozzle tip size 0.53–0.66 mm (21–26 thou); total paint pressure at the nozzle not less than 176 kg/cm² (2503 psi) |
|---|
| Air Spray | Suitable | Spray gun | DeVilbiss MBC or JGA |
| Air nozzle | 62 | ||
| (with pressure pot) | Spray painting | AC | |
| Brush | Suitable | For small areas and stripe coating only | |
| Roller application | Suitable | For small areas and stripe coating only | |
| Thinner | International GTA007 | Recommended maximum thinning ratio not to exceed 5%. Normally no thinning is required. |
In extreme cases, consult the local technical representative.
Do not thin beyond the requirements of local environmental regulations.
| Cleaner | International GTA007S. Select a cleaning agent compliant with local regulations. For specific usage recommendations, consult your local representative. |
|---|---|
| Interruption of work | Do not allow paint to remain in paint lines, spray guns or spray equipment. Thoroughly flush all equipment with International GTA007S. |
Once mixed, paint should not be resealed. If work is interrupted for too long, mix a fresh batch for application.
| Cleaning | All equipment should be cleaned immediately after use with International GTA 007S. Periodic flushing of spray equipment during the daily work process is a good practice. The frequency of cleaning depends on factors such as spray volume, temperature, spray time, including delays. |
|---|
All surplus paint and empty containers must be disposed of in accordance with the relevant local laws/regulations.
Airless spray application provides the highest film thickness in a single coat. When Interdur 8844 is applied by brush or roller, multiple coats are necessary to achieve the specified total system dry film thickness. If air spray is used, multiple cross coats are required to achieve maximum film thickness.
Apply under good weather conditions. The surface temperature to be coated must be at least 3 °C (5 °F) above the dew point. During the entire application and curing process, ensure adequate ventilation and air movement to prevent "dead corners"; especially when applying in confined spaces. In special cases, if recoating is required and the film has cured under low temperature and high humidity conditions, before applying the subsequent topcoat, ensure no amine
| salt is present. Condensation on the surface during or after application will lead to a matt surface and poor-quality film. | Premature exposure to standing water will cause colour change. Where a durable decorative surface with good gloss and colour retention is required, overcoat with the recommended topcoat. |
|---|
For atmospheric exposure, applied directly to steel, the minimum dry film thickness required for one coat is 350 µm (14 mils); for immersion service, the recommended minimum dry film thickness is 450 µm (18 mils). In both cases, a single coat can be applied by airless spray.
Interdur 8844 is suitable for steel structures under buried conditions (Im3 according to ISO 12944-2). Interdur 8844 can be used in conjunction with sacrificial anode and impressed current cathodic protection systems.
Note: VOC values are typical and for guidance only. They may vary with colour and general production tolerances.
Although the low-molecular-weight reactive additive becomes part of the film when cured under normal ambient conditions, analysis by EPA Method 24 shows that it also affects the VOC value.
For immersion service, Interdur 8844 is applied directly to steel.
For atmospheric exposure, the following primers are recommended for Interdur 8844: Intercure 200HS, Intergard 269, Interdur 8816, Interdur 8817, Interzinc 52, Intergard 251. Suitable topcoats are: Interdur 8860, Interfine 3399, Interfine 878, Intergard 740, Interthane 990.
| For further information on the industry standards, terms and abbreviations used in this datasheet, see www.international-pc.com | In the following documents on the website: • Definitions and abbreviations • Surface preparation • Coating application • Theoretical and practical spreading rate. These sections are also available as separate publications on request. |
|---|
Warning: this product contains liquid epoxy and modified polyamines and may cause skin sensitisation if handled improperly.
This product must be applied at the production site by professional applicators in accordance with the recommendations in this manual, the Material Safety Data Sheet and the instructions on the container label. Do not use this product without first reviewing the Material Safety Data Sheet (MSDS) that International Paint provides for its customers.
All work related to the application and use of this product must be carried out in accordance with the relevant national health, safety and environmental standards and regulations.
If welding or flame cutting is required on metal coated with this product, dust and fumes will be generated; use appropriate personal protective equipment and adequate local ventilation.
If in doubt about the suitability of this product for the intended use, consult AkzoNobel for further advice.
| Packaging Specifications | Component A | Component B | ||
| Volume | Packaging | Volume | Packaging | |
| 20 L | 16 L | 20 L | 4 L | 5 L |
For other packaging sizes, contact AkzoNobel.
| Packaging Specifications | Component A | Component B |
| 20 L | 30.1 kg | 4.5 kg |
| Shelf life | 12 months at 25 °C (77 °F). Thereafter, inspection is required. Store in a dry, cool environment away from heat and sources of ignition. |
|---|
© 2026/5/26 AkzoNobel. All rights reserved.
All registered trademarks mentioned in this publication are licensed to or owned by AkzoNobel.
www.international-pc.com
Information is subject to the manufacturer's latest version; the manufacturer's latest TDS prevails.
The technical parameters on this page are taken from the product's original manufacturer technical datasheet, the copyright of which belongs to the manufacturer. If a rights holder considers the presentation inappropriate, contact us for verification and handling.
Packaging specifications and batch lead times are subject to actual availability. PleaseContact Uscontact us for project-based calculation.