← Back to PPG brand page
China-based coatings exporter — industrial & marine protective coatings from China's production bases

PPG SIGMASHIELD 880GF AMERLOCK 880GF Abrasion-resistant Epoxy Coating 88

Quick Specs

PPG SIGMASHIELD 880GF AMERLOCK 880GF Abrasion-resistant Epoxy Coating 88 is an epoxy coating. Two-component surface-tolerant high-solids glass flake epoxy coating. Mainly used for maintenance protection of the splash zone on offshore platforms. Specifications on this page: volume solids 85 ± 2%, DFT 200-1000 µm (8.0-40.0 mil) depending on system requirements, theoretical spreading rate 4.3 m²/L. Comparable products of the same brand and type: AMERCOAT 114 A Epoxy Filler 114 A, AMERCOAT 240 SIGMACOVER 240 High-solids Multi-purpose Epoxy 240, AMERCOAT 370 Rapid-dry Multi-purpose Epoxy Coating 370.

Parameter source: PPG original technical data sheet (TDS) for PPG SIGMASHIELD 880GF AMERLOCK 880GF Abrasion-Resistant Epoxy 88; spreading rate and other values are converted from TDS parameters and provided for product selection reference only.
The above content is compiled from the manufacturer's datasheet and this site's parameter tables. For selection, coating systems and lead times, pleaseContact Usfor confirmation.

This page carries the full TDS for this product, translated from the manufacturer's original document. No file download is needed; for an original-language copy, send an enquiry.

Volume Solids85 ± 2%
Dry Film Thickness200-1000 µm (8.0-40.0 mil) depending on coating system requirements
Theoretical Spreading Rate4.3 m²/L
VOCMaximum 122.0 g/kg (EU Directive 1999/13…
Density / Specific Gravity1.5 kg/L (12.1 lb/US gal)
Number of ComponentsTwo-component
ThinnerThinner 91-92
Recoat IntervalMinimum: 3.5 h; maximum: 14 days

Browse Similar Models by CategoryThis model belongs to: Epoxy

IntroductionTwo-component, surface-tolerant high-solids glass flake epoxy

Key properties

Colour and gloss

Basic data at 20 °C (68 °F)

Parameters after mixing

Number of ComponentsTwo-component
Density1.5 kg/L (12.1 lb/US gal)
Volume solids85 ± 2%
VOC (as supplied)Maximum 122.0 g/kg (EU Directive 1999/13/EC, SED)

UK PG 6/23(92) Appendix 3: maximum 207.0 g/L (approx. 1.7 lb/US gal)

Recommended dry film thickness200-1000 µm (8.0-40.0 mil) depending on coating system requirements
Theoretical Spreading Rate4.3 m²/L at 200 µm (170 in²/US gal at 8.0 mil)
Touch Dry3 h
Recoat IntervalMinimum: 3.5 h; maximum: 14 days
Storage shelf lifeBase: at least 24 months; store in a dry and cool environment

Curing agent: at least 24 months; store in a dry and cool environment

Notes

Recommended substrate condition and temperature

Substrate condition

For maintenance projects, St2 of ISO 8501-1 or SSPC-SP2, or ultra-high-pressure water jetting to WJ2L/3L of UHPWH (SSPC-VIS-4) is required.

Substrate temperature and application conditions

Instructions for use

Mixing ratio by volume: base : curing agent = 75:25 (3:1)

Induction TimeNot required

Pot life after mixing

2 h at 20 °C (68 °F). Note: see supplementary parameters — pot life after mixing

Air spray

Recommended thinnerThinner 91-92
Thinner quantity4–8%, depending on the required film thickness and application conditions
Nozzle tip size1.5–3.0 mm (approx. 0.060–0.110 in)
Nozzle pressure0.2–0.4 MPa (approx. 2–4 atm; 29–58 psi)

Airless spray (single-feed pump)

Recommended thinnerThinner 91-92
Thinner quantity0-8%, depending on the required film thickness and application conditions
Nozzle tip sizeApprox. 0.53–0.69 mm (0.021–0.027 in)
Nozzle pressure15.0 MPa (approx. 150 atm; 2176 psi)

Brush/roller

Recommended thinnerThinner 91-92
Thinner quantity0 - 5%
Cleaning solventThinner 90-53

Supplementary parameters

Film thickness and spreading rate

Dry Film ThicknessTheoretical Spreading Rate
200 µm (8.0 mils)4.3 m²/L (170 in²/US gal)
500 µm (20.0 mils)1.7 m²/L (68 in²/US gal)

Recoat interval table for a coating at 500 µm (20.0 mils) dry film thickness

Subsequent coat for recoatingRecoat interval–5°C (23°F)5°C (41°F)10°C (50°F)20°C (68°F)30°C (86°F)40°C (104°F)
Self-recoatMinimum time36 h14 h7 h3.5 h2 h1.5 h
Maximum time2 months1.5 months1 month28 days21 days14 days
Overcoatable with various epoxy coatingsMinimum time36 h14 h7 h3.5 h2 h1.5 h
Maximum time1 month28 days21 days14 days7 days4 days
Recoat with polyurethane topcoatMinimum time48 h22 h14 h10 h6 h4 h
Maximum time1 month28 days21 days14 days7 days4 days
NotesThe surface must be clean, dry and free of all contaminants.

Curing time table for a coating at 500 µm (20 mils) dry film thickness

Substrate TemperatureSurface DryFully hard dryFully cured
-5 °C (23 °F)24 h48 h30 days
5 °C (41 °F)10 h24 h18 days
10 °C (50 °F)5 h16 h14 days
20 °C (68 °F)3 h8 h7 days
30 °C (86 °F)2 h5 h5 days
40 °C (104 °F)1 h3 h3 days

Notes

the final anticorrosive performance of the coating.

Pot life after mixing (at suitable application viscosity)

Mixed paint temperaturePot life after mixing
10 °C (50 °F)3 h
20 °C (68 °F)2 h
30 °C (86 °F)1 h

Safety Precautions

Worldwide

Although PPG Protective and Marine Coatings is committed to providing completely consistent products to users worldwide, from time to time it may be necessary to make minor adjustments to specific products to comply with local/national regulations or environmental requirements. In the following cases, use the corresponding alternative version of the product data sheet instead.

Reference information

Quality guarantee

PPG warrants (1) that it has good title to the product, (2) that the product quality conforms to the relevant technical quality specifications in force at the date of manufacture of the product, and (3) that the supplied product is free of lawful claims by third parties for infringement of US patent rights. The above warranties are limited to those given by PPG and other express or implied warranties required by applicable laws and regulations for transactions and commercial practice; any abuse contrary to the stated conditions, and any other warranty for special purposes or uses, are excluded, and PPG shall be free from liability. To claim under this warranty, the buyer must notify PPG in writing within five (5) days of discovering the quality defect, and the date must be within the product's valid storage period or within one (1) year from delivery of the product to the buyer.

If the buyer fails to notify PPG of the defect as required above, this will prejudice the buyer's right to obtain compensation under this warranty from PPG!

Limitation of liability

In all cases, PPG shall not be liable for any indirect, special, incidental or consequential loss of any kind arising from or in connection with the use of this product (whether based on negligence, strict liability or tort).

The information in this data sheet is derived from laboratory tests which we believe to be reliable, and is intended for reference and guidance only. As experience accumulates and product development continues, PPG may revise the information above at any time. All recommendations or suggestions regarding the use of this product, whether in technical documents, in reply to an enquiry or otherwise, are given to the best of our knowledge and the data is reliable. Our products and related information are provided for industrial users who have the necessary knowledge and practical skills; the end user of the product is responsible for determining whether the product is suitable for the specific purpose. Accordingly, the purchaser is assumed to have performed such evaluation and may act at its own discretion and risk.

The quality and condition of the substrate on site and the many other factors affecting the use and application of the product are beyond the control of PPG. Accordingly, PPG accepts no liability for any loss, injury or damage arising from the use of the information in this data sheet (except as otherwise provided in a separate written agreement). Different application environments, changes to the application process or speculation about the reference data may result in failure to achieve the expected coating quality.

This data sheet supersedes all previous editions. The purchaser is responsible for verifying, before using this product, that the data sheet in hand is the latest version. The current latest version is published on the official website of PPG Protective & Marine Coatings: www.ppgpmc.com. In the event of any discrepancy between the Chinese and English versions of this data sheet, the English original shall prevail.

The PPG Logo, Bringing innovation to the surface., and other PPG marks are property of the PPG group of companies. All other third-party marks are property of their respective owners.

FAQ

How many components is PPG?
PPG is a two-component product; mix in the ratio given in the Application Data table on this page before use.
What dry film thickness is typically applied for PPG?
The typical dry film thickness of PPG is 200-1000 µm (8.0-40.0 mil) depending on coating system requirements; the specific value is determined by the coating system and design requirements.
What is the theoretical spreading rate of PPG?
The theoretical spreading rate of PPG is 4.3 m²/L; the practical quantity is adjusted according to substrate roughness, application loss and colour hiding power.
What is the volume solids of PPG?
The volume solids of PPG is 85 ± 2%.
What is the VOC of PPG?
The VOC of PPG is a maximum of 122.0 g/kg (EU Directive 1999/13…
Which thinner is used for PPG?
Recommended thinner for PPG: Thinner 91-92.
Where can PPG be purchased?
RichTech Industrial Technology (Shanghai) Co., Ltd. distributes industrial and marine coatings; PPG PPG is one of our regularly stocked brands, with coating selection, system design and quantity calculation support. Address: 10F, Changhui Building, 799 Yinxiang Road, Jiading District, Shanghai, China. Tel: +86 21 5056 8299 (9:00–21:00).

Similar models from the same brand — epoxy coating

View all PPG models

Purchase & Documents

Packaging specifications and batch lead times are subject to actual availability. PleaseContact Uscontact us for project-based calculation.

China production baseIndustrial & marine coatingsWorldwide delivery